24 October 2026 Material selection 7 min read

Nobody buys Invar36 because it is easy to work with, and nobody buys it because it is cheap. You buy it because the mask is going to get hot, and you need the apertures to be in the same place when it is hot as they were when it was cold.

That single property — how much the material grows per degree — explains almost every material decision in this product. Everything else is secondary. This note puts the numbers side by side so you can decide from arithmetic rather than habit.

What actually happens when the mask heats up

In thermal evaporation the source radiates, the deposited film carries latent heat, and the mask warms. In sputtering the mask sees the plasma. In either case the mask does not stay at room temperature, and it rarely heats uniformly. Every degree of temperature change moves the aperture positions by an amount that depends only on the material and the distance across the part.

The arithmetic is simple. Expansion equals the coefficient of thermal expansion multiplied by the length multiplied by the temperature change. The interesting part is how large the result gets across a realistic mask size.

Growth of a 100 mm aperture array heated by 150 degrees Celsius
MaterialCTE (per °C)Growth across 100 mmRegistration risk
Invar361.2 × 10-618 µmLow
Molybdenum4.8 × 10-672 µmLow to moderate
Silicon reference2.6 × 10-639 µm—
Soda-lime glass reference9.0 × 10-6135 µm—
Stainless steel 31616.0 × 10-6240 µmHigh
Stainless steel 30417.3 × 10-6260 µmHigh

Two hundred and sixty microns is not a subtle error. On a device structure with 100 micron features it is two and a half features of drift. This is why a stainless mask can look perfect on the bench and produce visibly misaligned layers in the chamber.

Notice also that the correct comparison is not "which material moves least" but which material moves most like my substrate. A silicon wafer expands by 39 microns under the same conditions. Invar36 at 18 microns is much closer to silicon than stainless steel is, so the relative misregistration is far smaller even though neither is a perfect match.

Rule of thumb. Match the coefficient of thermal expansion of the mask to the substrate you are depositing onto, then check that the absolute movement stays inside your overlay budget. If the tolerances line up, use the cheaper material.

The four materials worth knowing

Invar36 (36% nickel iron, also called 4J36 or Alloy 36)

The standard answer whenever the mask sees heat and the features are fine. Coefficient near 1.2 × 10-6 per degree Celsius between 20 and 100 degrees Celsius, roughly one fourteenth that of 304 stainless. It photo-etches cleanly, which is how the fine apertures and burr free edges are produced. It is the default material for OLED research masks, perovskite evaporation masks and wafer level masks.

Three practical warnings. It is ferromagnetic, it rusts, and it stops being dimensionally special above roughly 230 degrees Celsius. All three are covered below.

Stainless steel 304 and 316

Cheap, readily available, etches beautifully, and tough enough to survive rough handling. Excellent for room temperature processes, front contact masks that never see significant heat, and mechanical fixtures. Also the right answer for magnetron sputtering, for the magnetic reason explained below.

316 is preferred if any wet chemistry or salt exposure is involved, since the molybdenum content improves pitting resistance.

Molybdenum

The high temperature answer. Coefficient near 4.8, and a melting point above 2600 degrees Celsius, so it stays stable long after Invar36 has lost its low expansion behaviour. Standard for high temperature evaporation sources and for processes with aggressive cleaning cycles between runs.

The tradeoffs are real. Molybdenum costs more per sheet, it is considerably harder to photo-etch, so feature limits are looser and the process costs more, and thin sections are brittle. It is not a casual upgrade, it is a decision made because the process demands it.

Nickel and copper

Nickel etches with excellent edge definition, which is why it shows up in fine mesh and precision sieve work, and it is used for electroformed masks where the apertures need near vertical walls. Coefficient near 13, so dimensionally it behaves like stainless rather than Invar. Copper is chosen when high thermal conductivity matters more than stability, for example to pull heat away from the substrate, and it also sputters cleanly.

Three cases where Invar36 is the wrong answer

1. Magnetron sputtering

Invar36 is ferromagnetic at room temperature, and its Curie point sits near 230 degrees Celsius. In a magnetron the plasma is confined by a magnetic field behind the target, and a ferromagnetic mask sitting in that field will distort it. The result can be shifted erosion tracks, changed deposition rates, and in bad cases unstable plasma. If the mask goes inside or near the magnetic circuit, choose annealed austenitic stainless steel 304 or 316, which are effectively non-magnetic.

This one trips up experienced people, because choosing Invar36 "for precision" is exactly the instinct that has the opposite effect here.

2. Processes running above about 250 degrees Celsius

Above the Curie point the alloy's low expansion anomaly disappears and its coefficient climbs towards ordinary steel values. You have paid the Invar36 premium and received stainless behaviour. Above roughly 250 degrees Celsius, molybdenum is the defensible choice.

3. Wet or corrosive environments

Invar36 contains no chromium. Despite the high nickel content, it is not stainless, and it will stain, pit and rust. Masks that get solvent soaked, acid cleaned, or simply stored in a humid cabinet will develop surface rust that transfers onto substrates and eventually degrades the aperture edges.

Handling rule for every Invar36 mask we ship: dry thoroughly after any wet step, and store wrapped in a low humidity cabinet. If the process genuinely involves standing liquids, move to 316 stainless or molybdenum.

Choosing by process instead of by material

Recommended starting point, then refine against your drawing
ProcessStart withWhy
Thermal evaporation, fine featuresInvar36Lowest drift as the mask heats
Electron beam evaporationInvar36 or molybdenumMoly if mask runs hot
Magnetron sputteringStainless 304 / 316Non-magnetic; does not distort the field
Sputter with heated substrateStainless 316Corrosion resistance plus stability
Above 250 °CMolybdenumInvar loses its advantage above Curie point
Room temperature contact printingStainless 304Cheapest that does the job
Wet chemistry involvedStainless 316 or molyInvar rusts
Perovskite single junction and tandemInvar36Evaporated transport layers need registration

What to tell us so the recommendation is reliable

  • Process — thermal evaporation, e-beam, or sputtering. Sputtering changes everything.
  • Peak mask temperature — measured if you have it, estimated if you do not.
  • Substrate material and size — silicon, glass, polymer. This sets the CTE to match.
  • Smallest feature and overlay budget — the tolerance you can actually live with.
  • Cleaning method between runs — solvent, ultrasonic, acid, or nothing.

Give us those five and we will recommend a material with the reasoning attached, including telling you when the cheaper option is genuinely fine. Full material data is also on the specifications page, and the material range is listed under products.

Frequently asked

What is the thermal expansion coefficient of Invar36?
Roughly 1.2 × 10-6 per degree Celsius between 20 and 100 degrees Celsius. Stainless steel 304 is about 17.3, roughly fourteen times higher. Above the Curie point near 230 degrees Celsius the alloy loses its low expansion behaviour and behaves much more like ordinary steel.
Is Invar36 magnetic?
Yes, it is ferromagnetic at room temperature and loses that behaviour near 230 degrees Celsius. In magnetron sputtering a ferromagnetic mask can distort the confining magnetic field. Annealed austenitic stainless 304 and 316 are effectively non-magnetic and are usually the safer choice in sputtering.
Does Invar36 rust?
Yes, and this surprises a lot of people. Invar36 has no chromium, so despite 36 percent nickel it is not stainless. Dry thoroughly after any wet cleaning and store wrapped in a low humidity cabinet, or move to 316 stainless if the process involves standing liquids.
When should I choose molybdenum instead?
Above roughly 250 degrees Celsius, or where aggressive cleaning between runs is routine. Molybdenum holds its low coefficient to far higher temperatures and resists cleaning chemistry, at the cost of higher material price, a harder etching process and brittleness in thin sections.